Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Ultramid® B3WG6 - PA6-GF30 - BASF

Material Data Center offers the following functions for Ultramid® B3WG6:
unit conversion, PDF datasheet print, comparison with other plastics, application examples, snap fit calculation, beam deflection calculation, parameters for material models, CAE Interfaces

Check here, which other Ultramid B datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Product Texts
Glass fibre reinforced and heat ageing resistant injection moulding grade used e.g. for automobile manifolds and pedals.
The products can also be offered as BMBcert™ and/or Ccycled™. Due to the Massbalance approach the product properties do not change.
Processing/Physical Characteristicsdry / condUnitTest Standard
ISO Data
Melt volume-flow rate, MVR 30 / * cm³/10min ISO 1133
Temperature 275 / * °C -
Load 5 / * kg -
Molding shrinkage, parallel 0.3 / * % ISO 294-4, 2577
Molding shrinkage, normal 0.8 / * % ISO 294-4, 2577
Thermal conductivity of melt 0.21 W/(m K) -
Spec. heat capacity of melt 2130 J/(kg K) -
Ejection temperature 160 °C -
Mechanical propertiesdry / condUnitTest Standard
ISO Data
Tensile Modulus 9500 / 6200 MPa ISO 527
Stress at break 185 / 115 MPa ISO 527
Strain at break 3.5 / 8 % ISO 527
Charpy impact strength, +23°C 95 / 110 kJ/m² ISO 179/1eU
Charpy impact strength, -30°C 80 / 85 kJ/m² ISO 179/1eU
Charpy notched impact strength, +23°C 15 / 30 kJ/m² ISO 179/1eA
Charpy notched impact strength, -30°C 11 / 10.2 kJ/m² ISO 179/1eA
Thermal propertiesdry / condUnitTest Standard
ISO Data
Melting temperature, 10°C/min 220 / * °C ISO 11357-1/-3
Temp. of deflection under load, 1.80 MPa 210 / * °C ISO 75-1/-2
Temp. of deflection under load, 0.45 MPa 220 / * °C ISO 75-1/-2
Vicat softening temperature, B 220 / * °C ISO 306
Coeff. of linear therm. expansion, parallel 25 / * E-6/K ISO 11359-1/-2
Coeff. of linear therm. expansion, normal 102 / * E-6/K ISO 11359-1/-2
Burning Behav. at 1.5 mm nom. thickn. HB / * class IEC 60695-11-10
Thickness tested 1.5 / * mm -
Yellow Card available yes / * - -
Oxygen index 22.5 / * % ISO 4589-1/-2
Electrical propertiesdry / condUnitTest Standard
ISO Data
Relative permittivity, 1MHz 3.8 / 6.8 - IEC 62631-2-1
Dissipation factor, 100Hz 230 / 2200 E-4 IEC 62631-2-1
Dissipation factor, 1MHz 230 / 2200 E-4 IEC 62631-2-1
Volume resistivity 1E13 / 1E10 Ohm*m IEC 62631-3-1
Surface resistivity * / 1E10 Ohm IEC 62631-3-2
Electric strength 41 / 31 kV/mm IEC 60243-1
Comparative tracking index - / 450 - IEC 60112
Other propertiesdry / condUnitTest Standard
Water absorption 6.6 / * % Sim. to ISO 62
Humidity absorption 2.1 / * % Sim. to ISO 62
Density 1360 / - kg/m³ ISO 1183
Material specific propertiesdry / condUnitTest Standard
ISO Data
Viscosity number 140 / * cm³/g ISO 307, 1157, 1628
Test specimen productionValueUnitTest Standard
ISO Data
Injection Molding, melt temperature 280 °C ISO 294
Injection Molding, mold temperature 80 °C ISO 294
Injection Molding, injection velocity 200 mm/s ISO 294
Processing Recommendation Injection MoldingValueUnitTest Standard
Pre-drying - Temperature 80 °C -
Pre-drying - Time 4 h -
Processing humidity ≤0.15 % -
Melt temperature 270 - 290 °C -
Mold temperature 80 - 90 °C -
Diagrams
Viscosity-shear rate , Ultramid® B3WG6, PA6-GF30, BASF
Shearstress-shear rate , Ultramid® B3WG6, PA6-GF30, BASF
Dynamic Shear modulus-temperature , Ultramid® B3WG6 (dry), PA6-GF30, BASF
Dynamic Shear modulus-temperature , Ultramid® B3WG6 (cond.), PA6-GF30, BASF
Stress-strain , Ultramid® B3WG6 (dry), PA6-GF30, BASF
Stress-strain , Ultramid® B3WG6 (cond.), PA6-GF30, BASF
Secant modulus-strain , Ultramid® B3WG6 (dry), PA6-GF30, BASF
Secant modulus-strain , Ultramid® B3WG6 (cond.), PA6-GF30, BASF
Stress-strain (isochronous) 23°C, Ultramid® B3WG6 (cond.), PA6-GF30, BASF
Creep modulus-time 23°C, Ultramid® B3WG6 (cond.), PA6-GF30, BASF
Creep curve 23°C, Ultramid® B3WG6 (cond.), PA6-GF30, BASF
Stress-strain (isochronous) 90°C, Ultramid® B3WG6 (dry), PA6-GF30, BASF
Creep modulus-time 90°C, Ultramid® B3WG6 (dry), PA6-GF30, BASF
Creep curve 90°C, Ultramid® B3WG6 (dry), PA6-GF30, BASF
Stress-strain (isochronous) 120°C, Ultramid® B3WG6 (dry), PA6-GF30, BASF
Creep modulus-time 120°C, Ultramid® B3WG6 (dry), PA6-GF30, BASF
Creep curve 120°C, Ultramid® B3WG6 (dry), PA6-GF30, BASF
Specific volume-temperature (pvT) , Ultramid® B3WG6, PA6-GF30, BASF
Tensile modulus-temperature , Ultramid® B3WG6 (dry), PA6-GF30, BASF
Tensile modulus-temperature , Ultramid® B3WG6 (cond.), PA6-GF30, BASF
Characteristics
Processing
Injection Molding
Delivery form
Pellets
Additives
Lubricants, Release agent
Special Characteristics
Heat stabilized or stable to heat
Regional Availability
Other text information
Injection molding
PREPROCESSING
Pre/Post-processing, max. allowed water content: .15 %
Pre/Post-processing, Pre-drying, Temperature: 80 °C
Pre/Post-processing, Pre-drying, Time: 4 h

PROCESSING
injection molding, Melt temperature, range: 270 - 290 °C
injection molding, Melt temperature, recommended: 280 °C
injection molding, Mold temperature, range: 80 - 90 °C
injection molding, Mold temperature, recommended: 80 °C
injection molding, Dwell time, thermoplastics: 10 min
Chemical Media Resistance
Acids
Acetic Acid (5% by mass) (23°C)
Application examples
Active intake manifold Audi A4
Air suspension piston
Housing, intake manifold
Intake manifold VW 1,8 Liter engine
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.